1. Home
  2. Resources
  3. Lead-free and DZR brass
Guide · CW511L · CW724R · CW602N

Lead-free and DZR brass

Standard free-cutting brass contains up to 3.5 % lead, and in some waters it loses zinc. Two families of grades deal with this: dezincification-resistant (DZR) brass, and low-lead or lead-free brass. Some grades are both.

Updated  · AirGrip, Jamnagar

What dezincification is

In some waters, zinc is drawn out of the brass and leaves a porous, weak copper layer behind. Fittings start to weep, threads lose strength, and white deposits appear on the outside. The zinc-rich β phase is attacked first, so ordinary two-phase free-cutting brass such as CW614N is the most exposed.

DZR grades combine a higher copper content with a small arsenic addition (0.02–0.15 %) and are often heat-treated after forging so that the structure resists the attack. Resistance is shown with the accelerated test in ISO 6509-1, which measures the depth of dezincification; the acceptance depth comes from the product standard or your specification.

The grades

Limits in % by weight. Zinc is the remainder.

GradeDesignationCuPbOtherDZRLow-lead
CW602NCuZn36Pb2As61.0–63.01.7–2.8As 0.02–0.15YesNo
CW511LCuZn38As61.5–63.5≤ 0.2As 0.02–0.15YesYes
CW724RCuZn21Si3P75.0–77.0≤ 0.10Si 2.7–3.5, P 0.02–0.10Depends on conditionYes
CW614NCuZn39Pb357.0–59.02.5–3.5—NoNo

CW614N for comparison. For CW724R, mills state dezincification resistance for defined conditions (some forging stock needs heat treatment after forging); call up the DZR test if you need it. Nearest equivalents: brass grade equivalents.

The rules behind them

Drinking water, EU. Materials in contact with drinking water fall under Directive (EU) 2020/2184. Its European positive list of metallic compositions (Implementing Decision (EU) 2024/367) applies from 31 December 2026. National schemes, such as the common composition list of the 4MS countries, have been the reference until then. Ask your certification body which compositions it accepts for your product type.

Drinking water, USA. Since 2014 the Safe Drinking Water Act allows a weighted average of at most 0.25 % lead on wetted surfaces of pipes, fittings and fixtures. Products are usually certified to NSF/ANSI 372.

Electrical and electronic equipment, EU. RoHS limits lead to 0.1 % by weight unless an exemption applies. Leaded brass uses exemption 6(c) (up to 4 % lead in copper alloys), currently valid until 30 June 2027. CW724R, with at most 0.10 % lead, meets the limit without it. CW511L allows up to 0.2 %, so check the heat analysis on the 3.1 certificate if you rely on it for RoHS.

Machining and cost

Without lead to break the chip, lead-free and low-lead grades form longer chips. They machine on the same cam automats and CNC lathes, with chip-breaking tool geometry, adjusted speeds and usually longer cycle times than CW614N. CW724R is also stronger, which is useful for thin walls but harder on tools.

Metal cost follows copper content: CW724R has about 76 % copper against 58 % in CW614N. Expect a higher piece price for lead-free parts, mostly from material and cycle time.

Which grade for which use

UseGrades to consider
Drinking-water fittings, EuropeA composition accepted for your product type; confirm with your certification body before ordering
Drinking-water fittings, USALead-free to the 0.25 % weighted-average rule, e.g. CW724R (nearest UNS C69300)
Water that attacks brass (soft, high-chloride), heating and marineDZR: CW602N or CW511L
Electrical parts that must not rely on RoHS 6(c)CW724R
Everything elseCW614N or CW617N: see CW614N vs CW617N

We run low-lead DZR CW511L, lead-free CW724R and DZR CW602N on request. Put the grade and standard on your drawing; the EN 10204 3.1 certificate that comes with every batch shows the heat analysis.

Questions

Is DZR brass lead-free?
Not necessarily. CW602N is DZR but contains 1.7–2.8 % lead. DZR is about corrosion; lead-free is about lead content. CW511L is both DZR and low-lead.
What is CW511L?
CuZn38As: a brass with 61.5–63.5 % copper, an arsenic addition for dezincification resistance and at most 0.2 % lead. Used for drinking-water fittings and parts for lead-restricted markets.
Is CW724R the same as C69300?
They are the nearest equivalents: both are silicon brasses with about 75 % copper and very low lead. Check the limits of the specification your drawing calls up.
Can lead-free brass be machined on normal machines?
Yes, on the same automats and CNC lathes, with chip-breaking tools and adjusted speeds. Cycle times are usually longer than with CW614N.
Which test shows that brass is DZR?
The accelerated dezincification test in ISO 6509-1. It measures the depth of attack; the acceptable depth is set by the product standard or by your specification.

Related

Need a lead-free or DZR part?

Send the drawing with the grade and the standard; we confirm material and certificate with the quote.